Adjustment Recommendation for Perfect Machine Cutting
Narrowing of kerf (divergent)
EN
Forward speed of torch
too fast
Distance between nozzle
and sheet metal too big
Dirty and / or damaged
nozzle
Concave cut surface profile
Forward speed of torch
too fast
Dirty and/or damaged noz-
zle or nozzle size too small
for the thickness to be cut
Cutting oxygen pressure
too low
Melted down top edge
with adherent slag
Cutting oxygen pressure
too high
Heating flame too strong
Distance between nozzle
and sheet metal too big
Single gouges
Forward speed of torch
too slow
Scaled or corroded or dirty
sheet metal surface
Distance between nozzle
and sheet metal too small
Flame too weak
Flame extinguished with
a ban
Sheet metal with finely
divided inclusions
Narrowing of kerf (conver-
gent)
Forward speed of torch
too fast
Distance between nozzle
and sheet metal too big
Cutting oxygen pressure
too high
Irregular cut surface profile
Cutting oxygen pressure
too low
Dirty and / or damaged
nozzle
Forward speed of torch
too fast
Lower edge rounded
Cutting oxygen pressure
too high
Forward speed of torch
too fast
Dirty and / or damaged
nozzle
Grouped gouge areas
Forward speed of torch
too fast
Scaled or corroded or dirty
shee metal surface
Distance between nozzle
and sheet metal too small
Flame too weak
Concave cut surface beneath
top edge
Cutting oxygen pressure
too high
Dirty and / or damaged
nozzle
Distance between nozzle
and sheet metal too big
Edge melting on
Forward speed of torch
too slow
Heating flame too strong
Distance between nozzle
and sheet metal too big to
too small
Nozzle size too big for the
thickness to be cut
Excessive cut drag line depth
Forward speed of torch too
fast or irregular
Distance between nozzle
and sheet metal too small
Heating flame too strong
Grouped gouges in the bot-
tom half of the cut
Forward speed of torch
too slow
Dirty and / or damaged
nozzle
14/136
Step at bottom edge
Forward speed of torch
too fast
Dirty and / or damaged
nozzle
String of solidified droplets
Heating flame too strong
Distance between nozzle
and sheet metal too small
Scaled or corroded sheet
metal surface
Excessive cut drag line
depth
Forward speed of torch too
fast or irregular
Distance between nozzle
and sheet metal too small
Heating flame too strong
Firmly adherent slag line
ad bottom edge
Forward speed of torch
too fast or too slow
Distance between
nozzle and sheet metal
too big
Cutting oxygen pressure
too low
Nozzle size too small for
the thickness to be cut
Flame too weak
Scaled or corroded or
dirty (colour) sheet metal
surface