▷ Steam off frame with steam cleaner (e. g. Steamer X3 (116910)).
▷ Oxidation firing is not necessary. Should an optical check neverthe-
less be desired, perform oxidation firing at 980 °C with 1 minute
dwell time. Afterwards, thoroughly blast off one more time.
Finish
▷ Gloss up metal edges using silicone polish. Prevent heat generation.
Laser welding
▷ Prepare connecting location in the form of a modified X seam.
▷ Blast off and clean the spot to be laser welded (using 110 - 250 μm
pure aluminium oxide).
▷ Use CoCr laser welding wire (721130 ff).
After laser welding the Ceramill Sintron, the workpiece can be
ceramic veneered.
Soldering
▷ Solder using CoCrMo filler (781630 Girosolder) and the correspond-
ing flux.
After soldering the Ceramill Sintron, the workpiece can be ceramic
veneered.
Veneer ceramics
As a general rule, all conventional metal veneer ceramics can be used.
▷ Observe and adhere the respective manufacturer's information!